Effect of intercritical annealing temperature on formability and bake-hardening-index of high strength steel for exposed auto body
The theoretical prediction of main strengthening elements,final hot rolling,coiling and intercritical annealing soaking temperature were conducted by thermodynamic calculations,which agreed with the experimental results.The good formability and bake-hardening-index property gained from the experimental procedure according to the calculations show that,n (tensile strain hardenability value),r (plastic strain ratio) and BH2 (bake-hardening-index) represent maximum value when soaking temperatures were set from 800 to 820℃,the maximum value ofn is 0.21,r is 1.39,BH2 is 44 MPa.
Formability Bake-hardening-index Intercritical annealing temperature
Fang FANG Fang-yi SUN Li-xin WANG
Research and Development Center, Wuhan Iron and Steel Co., Wuhan, China
国际会议
香港
英文
92-96
2012-12-11(万方平台首次上网日期,不代表论文的发表时间)